Recover Tungsten, Vanadium, Titanium from Waste SCR Catalyst 1/2

Due to denitration agents take 30%~50% the whole investment of denitration equipment in the system, besides the main component V2O5 is of highly toxic which will cause environmental pollution and poison to human body. So, it will create great economic and environmental benefits by comprehensive recycling waste catalyst. A method for recycling tungsten, vanadium and titanium from waste SCR catalyst is put forward in this paper, steps are as follows:

Waste SCR catalyst

1. SCR waste catalyst pretreatment, high temperature and pressure leaching out
1) Crushing and grinding the waste catalysts, then send them to NaOH solution which the concentration is 200~700g/L, and then leaching out at high temperature (130~220℃), high pressure (0.3~ I.2MPa) for I~6 hours, get filtrate and residue;
Remarks: residue can be used as the material of Rutile Titanium Dioxide;
2) Add hydrochloric acid to adjust the pH value to 0.5~I.5, and heated to 90~100℃ to make Na4TiO4 reacted to H4TiO4, then filter for getting filtrate and residue;
Remarks: ①. Filtrate and washed wastewater are joined into reuse process of wastewater;
②. The residue after washing is calcined at the temperature of 800~900℃ for 2-4 hours to get Rutile Titanium Dioxide.
2. Adjust pH by adding hydrochloric acid to remove impurities
Add hydrochloric acid into leaching solution which is got from step 1 to adjust pH value to 10~11, then add MgCl2 for removing impurity; concentrate and again add hydrochloric acid to adjust pH value to 9~10, and then precipitate WO42- and VO3- ions, separate to obtain filtrate and filter residue, the filter join into reuse process of wastewater.

 

 

WeChat