1) The electroforming process uses a DC power supply voltage: 3 V to 15 V, current density: 1 ~ 12A/dm2, the anode and the cathode are inserted in the electroforming solution, pure nickel is an anode, while a cathode is stainless steel or Ti ;
2) The composition of the electroforming solution of nickel sulfamate: 120 to 350 g / l, nickel chloride: 20 ~ 45 g / l, sodium tungstate: 480 ~ 1400 g / l, boric acid: 10 ~ 50 g / l . In the electroforming process, we should stire, the stirring speed: 60 to 130 rev / min;
3) Electroforming process performed at a constant temperature is 550C, then the filtration residue, electroforming process control time: 1 hour to 12 hours.
Advantage of the present invention is that: the Ni atom, and W atoms in each electric crystal grains was occupied by each gap arrangement, succeeded in preparing high density tungsten-nickel alloy block.